O, N determination in titanium samples

阅读:5544      发布时间:2015-5-15
分享:
  Suitable analyzers
n ON 900
n ONH 2000
Used accessories
n Inner graphite crucibles (90180)
n Outer graphite crucibles (90185)
n Nickel basket (90250) or AR 2344
n Suitable calibration material (NIST or other)
Settings
n Comparator level: 20 mV
n Minimum time: 15 sec
n Maximum time: 3:00 min
n Post waiting: 30 sec
n Base line deviation: 200 mV;
Step: 16 mV; Time: 10 sec
n Mode: continuous
n Outgas
Time: 45 sec
Power: 6 kW
n Time
Purge: 20 sec
Stability: 45 sec
n Integration delay
IR cell: 2 sec
TC cell: 10 sec
n Analyse (1)
Time: 75 sec
Power (1): 6 kW
Power (2): 6 kW

Sample preparation
Make sure that the surface of the titanium is free
from contaminations; otherwise clean the sample with
acetone p.a. and let dry at atmosphere.
Procedure
n Prepare ELTRA analyzer (exchange anhydrone,
sodium hydroxide, copper oxide when necessary),
clean furnace, sample drop mechanism, electrode tip
n Run three blanks with empty crucibles
n Calibrate the analyzer with suitable calibration
material (NIST or other)
(1) Fill one empty inner crucible (90180) in one outer
crucible (90185) and place them on the electrode
tip, close furnace (F2 Button)
(2) Weigh calibration material and give it into a nickel
basket (90250 or AR2344)
(3) Place nickel basket with calibration material or sample
in the sample drop mechanism and start analysis
(F5 Button)
After analysis give the inner crucible into waste and
fill in a new one. The outer crucibles can be used
approximay 10 times.
Repeat steps (1) – (3) at least three times;
Mark the results and use the calibration function in the
software.


提供商

弗尔德(上海)仪器设备有限公司

下载次数

195次

资料大小

370KB

资料类型

PDF 文件

资料图片

--

浏览次数

5544次

产品展示

会员登录

请输入账号

请输入密码

=

请输验证码

收藏该商铺

标签:
保存成功

(空格分隔,最多3个,单个标签最多10个字符)

常用:

提示

您的留言已提交成功!我们将在第一时间回复您~
在线留言