C, S determination in ore samples

阅读:2575      发布时间:2015-5-15
分享:
  Suitable analyzers
n CS-800
n CS-2000 (induction furnace)
Used accessories
n Ceramic crucibles (90150)
n Tungsten (90220)
n Iron accelerator (90260)
n Suitable calibration material (NIST or other)
Settings
n Comparator level: 20 mV
n Minimum time: 40 sec
n Maximum time: 3:00 min
n Integration delay: 6 sec
n Post-waiting: 15 sec
n Pre-purging: 10 sec
n Base line deviation: 10 mV
Base line time: 15 sec
n T1 - Pre-purging: 5 sec
n T2 - Chamber only: 5 sec
n T3 - Chamber and lance: 3 sec
n T4 - Generator: 45 sec

Sample preparation
For best results grind the sample down to a particle size of approx. 200 µm.
Dry the sample to constant mass at 105°C (at least 1 hour).
Pre-heating the crucibles (1 h; 1000°C) could improve the precision.
Procedure
n Prepare ELTRA analyzer (e.g. exchange anhydrone, sodium hydroxide,
copper oxide when necessary); clean the combustions tube
n Run three warm up samples (e.g. steel samples (92400-3050) with a
minimum weight of 500 mg; add 1.5 g tungsten)
n Calibrate the analyzer with suitable calibration material (NIST or other)
(1) Weigh in 150 mg of sample in the ceramic crucibles (90150)
(2) Add 0.7 (±0.1) g of iron accelerator (90260) and 2.0 (±0.1) g of
tungsten (90220)
(3) Place the crucible on the pedestal and start analysis
Repeat Step (1) – (3) at least three times;
Mark the results and use the calibration function in the software.


提供商

弗尔德(上海)仪器设备有限公司

下载次数

231次

资料大小

347.4KB

资料类型

PDF 文件

资料图片

--

浏览次数

2575次

产品展示

会员登录

请输入账号

请输入密码

=

请输验证码

收藏该商铺

标签:
保存成功

(空格分隔,最多3个,单个标签最多10个字符)

常用:

提示

您的留言已提交成功!我们将在第一时间回复您~
在线留言